HI All
it reall does depend what equipment you using Start with 3m Trizact
A45 (320) Then 3m Trizact A16 (1000) Then sisal mop with green bar
compound -then stitched cotton mop with white bar compound -then
swans down loose leaf mop with rouge or the finest you can get.
Remember if you put a scratch in it you have to take it out else it
is going to be highlighted when you get to the mirror finish. So take
more time with the A45 AND A16 you will be rewarded in the end. also
do not polish all in the same direction. do the first lengthways
then the next step at right angles to the first.
it will highlight all the scratches and you can proceed with ease
until they are all out. then the same with compounds etc etc. Satin
finishes are better for stainless as it scratches easy then your
mirror finish is marred.?